Difference between revisions of "Ball mill work index adjustment"
(→Ball mill work index adjustment) |
|||
Line 10: | Line 10: | ||
The precise method used to do the adjustment is based on [[Bibliography: Testwork programs|Josephin & Doll (2018)]]. |
The precise method used to do the adjustment is based on [[Bibliography: Testwork programs|Josephin & Doll (2018)]]. |
||
+ | * Compute K values for each grindability result: |
||
+ | <math>K = \frac{10 \times Wi_{test} \times (P_{80|test}^{-0.5} - F_{80}^{-0.5})}{P_{80|test}^{-a}}</math> |
||
+ | * Then compute the adjusted work index each grindability result using the ''K'' value: |
||
+ | <math>Wi_{adjusted} = \frac{K_{test} \times P_{80|adjusted}^{-a}}{10 \times (P_{80|adjusted}^{-0.5} - F_{80}^{-0.5})}</math> |
||
+ | |||
===Comments=== |
===Comments=== |
||
* When doing Bond/Barratt models, enter the exponent ''a'' into the '''Ball mill Wi adjust exponent (a)''' (drop the negative sign, ''a'' should always be positive when you enter it). |
* When doing Bond/Barratt models, enter the exponent ''a'' into the '''Ball mill Wi adjust exponent (a)''' (drop the negative sign, ''a'' should always be positive when you enter it). |
Revision as of 21:44, 10 April 2020
Ball mill work index adjustment
The Bond ball mill work index test requires the operator to select an appropriate screen size to "close" the test. The procedure states that the closing screen size should be such that the product size of the test is the same as the expected product size of the operating plant. If the tests were done at the wrong closing screen size, then a ball mill work index adjustment procedure can be conducted as follows:
- In the laboratory, select a series of samples, each suitable for performing three or more work index tests (probably 30 kg of sample is the practical minimum).
- Conduct a series of work index determinations on each sample, but vary the closing screen mesh. At minimum, test two different closing mesh sizes (the closing size you did the original tests at, and the closing size that matches your new desired P80). Three or four different mesh sizes are better.
- Calculate the specific energy of each ball mill test, Eball = 10 × Wi (P80-0.5 - F80-0.5)
- Fit the specific energy results for all BM tests, Eball = K × P80-a. Use the power regression model or use logarithms to rearrange and solve for a and K using linear regression of the logarithms.
- If there is a clear discontinuity in the work index at a particular size, this probably indicates a hard grain size is being encountered in the test. If this grain size is between your original test P80 and the desired, P80, just continue with the procedure. If this grain size is above or below the size range of interest, then exclude those sizes and repeat the regression.
The precise method used to do the adjustment is based on Josephin & Doll (2018).
- Compute K values for each grindability result:
- Then compute the adjusted work index each grindability result using the K value:
Comments
- When doing Bond/Barratt models, enter the exponent a into the Ball mill Wi adjust exponent (a) (drop the negative sign, a should always be positive when you enter it).
- If using Morrell Mi models, then this adjustment doesn't apply (but you should do a manual check, Mib is usually very sensitive to P80).
- This adjustment only applies to regular Bond ball mill work index tests. The model will ignore the adjustment for any sample identified as a "modified ball mill test" (the ModBWI is set to a non-zero number).